This product is used in acidic etching to manufacture pattern graphics such as mirror steel, titanium steel, circuit board circuit, etc. It can be dried at room temperature and specially formulated for metal plate production. The ink has high viscosity, high thixotropy, good printing performance, no bubbles in the coating film, pinholes and patterns, and has good resistance to nitric acid, sulfuric acid, hydrochloric acid and other acid etchants after film formation, and is suitable for 180-360 meshes. Web printing. Since alkali caustic agent is used in the ink, the dilute alkali solution deinking film can be easily used after the etching process is completed, thereby greatly improving the work efficiency and safety of the processing plant.
Technical characteristics
Color: Black (BK)
Viscosity: 4.0 to 10.0 (25°C, Pa·S)
Fineness: ≤15
Drying conditions: 30 to 60 minutes at room temperature, heating and drying (80°C) for 3 to 5 minutes
Pencil hardness: ≥2H
Etching resistance: Etchants such as nitric acid, sulfuric acid, and hydrochloric acid
Remove film: 1~3% NaOH solution for 30~60 seconds
Storage stability: 1 year
Precautions:
1. The main solvent of this product is cyclohexanone or 783 thinner. Do not use alcohols or aqueous solvents.
2. It is best to use a thinner to clean the surface before printing.
3, before entering the strong acid corrosion must be detected whether the ink is dry and thorough.
4. Fireworks are strictly prohibited during printing.
Packing specification: 5kg 20kg
Suggested selling price: 120 yuan/kg
Strong acid etching ink formula
First, antacid resin liquid formula:
Material ratio Origin
Paint asphalt 25 Karamay oil field
Anti-acid resin 15 members see the registered e-mail
783 Thinner 60 Around Screen Shop
Production Process:
First, add 783 thinner in proportion, start stirring, heat (at 60 °C), and then put paint bitumen and antacid resin in turn, until completely dissolved. Filter for use.
Second, the finished product formula:
Material ratio Origin
Anti-acid resin liquid 60 See above
Alkaline collapse agents 25 027-87643278
783 Thinner 15
Production Process:
According to the above formula, the material is put into the mixing tank and stirred well, and then it is ground to a fineness of 20 microns or less using a sand mill. Qualified after the package.
Source: China Ink Technology Network